Boiler Industry Coating Material

Boiler Industry  Coating Material: 76MXC bond coat under a thermal barrier

 

 

Protective Tube

Problem: high temperature corrosion

 

Solution:  8830 Arc Spray System with ArcJet

 

Coating Procedure:

 

Preparation method: Grit blast with aluminum oxide, 40 mesh  at 100 psi [690  kPa]

Spray parameters: 175 Amps, 30 volts, 20 lbs [9.07 kg]/hr

Spray Time: 40 minutes

Spray angle:  90ー

Coating thickness: .020" [.508 mm]

Preheat temperature: 100ーF [38ーC]

Temperature during spray: 400ーF [204ーC]

Lathe speed: 550 rpm

Traverse speed: 215 sf/m

Base metal: Heat treated steel

Amount of material used:  6 pounds [2.7 kg] of 76MXC

 

Finishing Procedure:

Method:  none

Finished thickness: .020" [.51 mm]

Sealer used: none